VIETSOVPETRO
DOCUMENT TITLE: STRUCTURAL WELD PROCEDURE SPECIFICATION
PROPOSAL
DOCUMENT No: VSP – MEO – 01S(2G-3G-4G)
0 21/12/09 For Review
REV DATE DESCRIPTION PREPARED BY CHECKED BY APPROVED BY
Page 1 of 3
WELDING PROCEDURE DOC. No:VSP-MEO-01S(2G-3G-4G)
SPECIFICATION PROPOSAL REV. No: 0
VIETSOVPETRO DATE : 21/12/2009
CODE/ STANDARD : AWS D1.1-2008
WPS No: VSP-MEO-01S(2G-3G-4G) Rev: 0 Date : 21/12/2009
Supporting PQR No: PQ.SM-01S (2G) Date :
PQ.SM-02S (3G) Date :
PQ.SM-03S (4G) Date :
Welding Process: SMAW Type: Manual
JOINTS:
Joint Design: CJP Single Vee
Backing: N/A
Backing Material Type: N/A
Back Gouging: N/A
Method: N/A
Root gap 3.5 0.5mm
Root Face: 1.6 0.5mm
Angle Groove: 60 5
BASE METALS:
Test material Spec: ASTM – A572
Type or Grade: Gr 50
Test Dimension: Plate 10mm
Qualified Material: Group I To Group I, Group I To Group II, Group II To Group II
(Table 3.1& Table 4.8 AWS D1.1)
Range :
Thickness : 3mm to 20mm Fillet: All
Diameter (Pipe ) : 600 mm and Over Fillet: All
FILLER METALS: SMAW
F No: 4
A No: 1
SFA No: 5.1
AWS No (Class): E7016 / E7018
Size of Filler Metals ( mm ): 3.2, 4.0
Electrode Flux Class: N/A
Flux Trade Name: N/A
Electrode /Wire Trade Name: LB52U-KOBELCO
Page 2 of 3
WELDING PROCEDURE DOC. No:VSP-MEO-01S(2G-3G-4G)
SPECIFICATION PROPOSAL REV. No: 0
VIETSOVPETRO DATE : 21/12/2009
POSITIONS QUALIFIED POST WELD HEAT TREATMENT
Position of Groove: All (except 6GR) Temperature Range: N/A
Welding Progression: Up hill Thickness Range: N/A
Position of Fillet: All Time interval: N/A
PREHEAT GAS :
Preheat Temp. Min.: Ambient Shielding Gas: N/A
Interpass Temp. Max: 250 deg.C % Composition: N/A
Preheat Maintenance: N/A Flow Rate: N/A
Temp. Check: Tempstick or Thermometer Purging Rate: N/A
ELECTRICAL CHARACTERISTICS :
Current AC: NA SMAW: DCEP
Tungsten Electrode Size & Type: N/A
Mode of Metal Transfer for GMAW: N/A
Electrode Wire Feed Speed Range: N/A
TECHNIQUE :
String or Weave Bead: String Or Weave max. 3 times of the electrode diameter
Orifice Or Gas Cup Size: N/A
Initial & Interpass Cleaning: Grinding/Brushing/Chipping
Method of Back Gouging: NA
Multi-pass or Single Pass (per side): Multipass
Other: N/A
INSTRUCTION
Thickness of thickest part of base metal (mm) Minimum preheat and interpass Temp. C
Group I Group II
4.8 To 38 Incl. 4.8 To 19 Incl. Ambient
Over 38 To 63.5 Incl. Over19 To 38 Incl. 66
WELDING VARIABLE
Filler Metal Welding Current Travel
Weld Heat Input
Process Volt Speed
Layers Class Dia.(mm) Type Amps (KJ/mm)
(mm/min.)
Root SMAW E7016 3.2 DCEP 75-95 19 -21 51 - 65 1.31-2.35
Rest/Cap SMAW E7018 3.2 DCEP 85-130 22-26 70-120 0.935-2.89
Rest/Cap SMAW E7018 4.0 DCEP 120-170 22-26 100-160 0.99-2.65
Prepared By: Checked By: App. By VSP: App. By CA:
Signature: Signature: Signature: Signature:
Date : Date : Date : Date :
Page 3 of 3