Able 1-Chemical Composition of Material Used, WT%: Elements Base Materials Inconel C-22 Undiluted Filler Materials

The document contains 5 tables that provide information on the chemical composition, welding parameters, mechanical properties, impact energy values, and hardness values of Inconel 276, Inconel 617, and Inconel C-22 materials. Table 1 details the chemical composition of each material in weight percent. Tables 2 and 3 list the gas tungsten arc welding parameters and tensile properties measured. Table 4 reports the charpy v-notch impact energy values and failure locations. Table 5 gives the maximum and average Vickers hardness numbers.

Uploaded by

Sayiram G
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as DOCX, PDF, TXT or read online on Scribd
0% found this document useful (0 votes)
78 views5 pages

Able 1-Chemical Composition of Material Used, WT%: Elements Base Materials Inconel C-22 Undiluted Filler Materials

The document contains 5 tables that provide information on the chemical composition, welding parameters, mechanical properties, impact energy values, and hardness values of Inconel 276, Inconel 617, and Inconel C-22 materials. Table 1 details the chemical composition of each material in weight percent. Tables 2 and 3 list the gas tungsten arc welding parameters and tensile properties measured. Table 4 reports the charpy v-notch impact energy values and failure locations. Table 5 gives the maximum and average Vickers hardness numbers.

Uploaded by

Sayiram G
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as DOCX, PDF, TXT or read online on Scribd
You are on page 1/ 5

able 1-Chemical composition of material used, wt%

Undiluted filler materials


Base Materials
Elements
Inconel C-22
Inconel 617
Inconel C-276

Ni 64.51 51.02 54.1


Cr 22.5 16.5 22.3
Fe 6 7 1.5
C 0.010 0.010 0.15
Mn 0.50 1.0 1.0
Si 0.08 0.08 1.0

Mo 14.5 17 8.8

W 3.5 4.5 -

Co 2.5 2.5 8

V 0.35 0.35 -

P 0.025 0.025 0.03

S 0.015 0.010 0.015

Cu - - 0.5

Ti - - 0.6

Al - - 1.5

B - - 0.005

1
Table 2-GTAW welding parameter

Welding parameters Total Heat


Pass Heat input
Filler input
Number (kJ/cm)
material Current Voltage Welding Speed (kJ/cm)
(A) (V) (cm/min)
Inconel
1 110 10 10 6.6
276
2 130 12 10 9.36
3 130 13 10 10.14
4 130 14 10 10.92 37.02
Inconel
1 110 10 10 6.6
617
2 130 12 10 9.36
3 130 13 10 10.14
4 130 14 10 10.92 37.02

2
Table 3 -Tensile properties of transverse specimens at room temperature (23◦C).

Ultimate tensile
Total Elongation Reduction in area
Metals strength Location of failure
(%) (%)
(Mpa)

Inconel 276 750 53 23 Weld Metal

Inconel 617 720 51 26 Weld Metal

Inconel C-22 690 45 25 -

3
Table 4–Charpy V notch impact energy value

Metals Impact Energy Failure location Type of failure

As-weld condition(J)

136 weld Ductile failure


Inconel 276

117 weld Brittle failure


Inconel 617

90 - -
C-22

4
Table 5-Hardness Value of the specimens at room temperature (23◦C)

Maximum Hardness Average Hardness


Metals
(VHN) (VHN)

Inconel 276 238 231

Inconel 617 241 215

C-22 225 213